欢迎访问《现代矿业》杂志官方网站,今天是 分享到:
×

扫码分享

现代矿业 ›› 2026, Vol. 42 ›› Issue (09): 106-112.

• 矿物加工工程 • 上一篇    下一篇

基于响应面法的某高纯磁铁矿精矿制备工艺优化

宛 鹤1 和 逸1 张 月2 张 雷2   

  1. 1. 西安建筑科技大学资源工程学院;2. 陕西华光实业有限责任公司
  • 出版日期:2026-09-25 发布日期:2026-10-10

Optimization of Preparation Process of a High Purity Magnetite Concentrate Based on Response Surface Method

WAN He¹ HE Yi¹ ZHANG Yue² ZHANG Lei2   

  1. 1. School of Resources Engineering,Xi'an University of Architecture and Technology; 2. Shaanxi Huaguang Industrial Co.,Ltd.
  • Online:2026-09-25 Published:2026-10-10

摘要: 为实现细粒磁铁矿精矿的高纯化制备,针对细粒磁铁矿精矿高纯化过程中存在的矿 物解离不充分、微细粒团聚明显、磁性夹带严重及脉石杂质难以深度脱除的问题,以陕西某选钼尾 矿磁选精矿为研究对象,进行了磨矿—分散协同参数优化及多工序磁选提质工艺试验,试验采用 响应面法优化磨矿—分散协同调控参数,并系统探究了消磁、脱泥、磨矿细度及梯度磁选次数对磁 选提质效果的影响。研究得到了各工艺参数的作用规律及最优工艺条件,PAA 用量、分散时间和 磨矿时间对精矿铁品位及铁回收率均具有显著影响,参数间存在明显交互作用;在确定的最优工 艺参数 PAA 用量 500 g/t、分散时间 3 min、磨矿时间 3 min的条件下,矿浆分散状态稳定,可有效抑制 脉石夹带。单一工艺优化试验结果显示:消磁处理可削弱磁团聚效应,将精矿铁品位由 70.0% 提升 至 70.8%;脱泥处理可去除微细粒云母、石英及含铁硅酸盐等泥质杂质,使精矿铁品位由 69.1% 提 升至 70.8%;当磨矿细度为-23 μm95.0% 时,可获得铁品位 70.80%、铁回收率 91.49% 的精矿产品; 采用 39.79,35.81,31.83 kA/m 的三段梯度磁选流程后,精矿最高铁品位可提升至 71.6%。响应面法 能够有效揭示磨矿—分散—磁选参数之间的协同作用关系,构建的消磁—磨矿—PAA 分散—脱 泥—三段梯度磁选工艺可有效实现细粒磁铁矿精矿提质,可为细粒磁铁矿高纯化制备提供可靠的 技术参考。

关键词: 高纯磁铁矿精矿, 响应面法, 磨矿细度, 分散调控, 消磁, 脱泥, 梯度磁选

Abstract: In order to realize the high-purity preparation of fine-grained magnetite concentrate,aim⁃ ing at the problems of insufficient mineral dissociation,obvious agglomeration of fine particles,serious magnetic entrainment and difficult deep removal of gangue impurities in the high-purity process of fine�grained magnetite concentrate,the magnetic separation concentrate of molybdenum tailings in Shaanxi Province is taken as the research object,and the grinding-dispersion synergistic parameter optimization and multi-stage magnetic separation quality improvement process test are carried out.The response surface method is used to optimize the grinding-dispersion synergistic control parameters,and the effects of demag⁃ netization,desliming,grinding fineness and gradient magnetic separation times on the quality improvement of magnetic separation are systematically investigated.The action law of various process parameters and the optimal process conditions are obtained. The amount of PAA,dispersion time and grinding time have signifi⁃ cant effects on the iron grade and iron recovery of the concentrate,and there are obvious interactions be⁃ tween the parameters.Under the determined optimal process parameters of PAA dosage of 500 g/t,dispersion time of 3 min and grinding time of 3 min,the slurry dispersion state is stable,which can effectively inhibit the entrainment of gangue. The results of single process optimization test show that demagnetization treat⁃ment can weaken the magnetic agglomeration effect and increase the iron grade of concentrate from 70.0% to 70.8%.Desliming treatment can remove argillaceous impurities such as fine mica,quartz and iron-con⁃ taining silicate,and increase the iron grade of concentrate from 69.1% to 70.8%. When the grinding fineness is -23 μm95.0%,the concentrate product with iron grade of 70.80% and iron recovery of 91.49% can be ob⁃ tained.After adopting the three-stage gradient magnetic separation process of 39.79,35.81,31.83 kA/m, the highest iron grade of the concentrate can be increased to 71.6%. The response surface method can effec⁃ tively reveal the synergistic relationship between grinding-dispersion-magnetic separation parameters. The constructed demagnetization-grinding-PAA dispersion-desliming-three-stage gradient magnetic separa⁃ tion process can effectively realize the quality improvement of fine-grained magnetite concentrate,which can provide a reliable technical reference for the high-purity preparation of fine-grained magnetite.

Key words: high purity magnetite concentrate, response surface method, grinding fineness, disper? sion control, demagnetization, desliming, gradient magnetic separation