提高武山铜矿细粒黄铁矿回收率试验研究

武山铜矿选矿厂一段旋流器溢流硫品位为 8.46%,且粒度极细,-10 μm 粒级产率达
44.93%、硫分布率达44.20%。为提高现场细粒硫回收效果,进行了选矿试验研究。结果表明,二次分
级旋流器适宜的溢流管、沉砂嘴直径分别为 48、20 mm,二次分级沉砂硫分配率为 73.40%,较现场旋
流器参数下提高 2.13个百分点;试验确定的捕收剂乙基黄药粗选总用量为 140 g/t,对应的粗选 1、扫
选1、扫选2用量分别为80、40、20 g/t;试样的旋流器分级沉砂采用1粗2扫、中矿合并返回流程处理,
与中矿顺序返回流程相比,在精矿硫品位略低的情况下硫回收率提高了1.7个百分点;将现场细粒浮
选2次扫选精矿合并给入粗粒浮硫扫选2作业,可提高硫回收率1.4个百分点,工业试验指标较好。
  

  1. 江西铜业股份有限公司武山铜矿
  • 出版日期:2024-02-18 发布日期:2024-08-14

Experimental Study on Improving the Recovery Rate of Fine-grained Pyrite
in Wushan Copper Mine

The sulfur grade of the first-stage cyclone overflow in the concentrator of Wushan Copper
Mine is 8.46%,and the particle size is extremely fine. The yield of -10 μm particle size is 44.93%,and the
sulfur distribution rate is 44.20%. In order to improve the effect of on-site fine sulfur recovery,a beneficia⁃
tion test was carried out. The results show that the suitable diameters of the overflow pipe and the grit nozzle
of the secondary classification cyclone are 48 mm and 20 mm respectively,and the sulfur distribution rate of
the secondary classification grit is 73.40%,which is 2.13 percentage points higher than that of the on-site
cyclone parameters. The total amount of collector ethyl xanthate determined by the test was 140 g/t,and the
corresponding amounts of roughing 1,scavenging 1 and scavenging 2 were 80,40 and 20 g/t,respectively.
The cyclone grading grits of the sample were treated by one roughing two scavenging and middling merging
and returning process. Compared with the middling sequential returning process,the sulfur recovery rate
was increased by 1.7 percentage points under the condition of slightly lower sulfur grade of the concentrate.
The on-site fine-grained flotation two-time scavenging concentrate is combined into the coarse-grained sul⁃
fur flotation two-time scavenging operation,which can increase the sulfur recovery rate by 1.4 percentage
points,and the industrial test index is good.
  

  1. Wushan copper mine,Jiangxi Copper Co.,Ltd.
  • Online:2024-02-18 Published:2024-08-14

摘要:

武山铜矿选矿厂一段旋流器溢流硫品位为 8.46%,且粒度极细,-10 μm 粒级产率达
44.93%、硫分布率达44.20%。为提高现场细粒硫回收效果,进行了选矿试验研究。结果表明,二次分
级旋流器适宜的溢流管、沉砂嘴直径分别为 48、20 mm,二次分级沉砂硫分配率为 73.40%,较现场旋
流器参数下提高 2.13个百分点;试验确定的捕收剂乙基黄药粗选总用量为 140 g/t,对应的粗选 1、扫
选1、扫选2用量分别为80、40、20 g/t;试样的旋流器分级沉砂采用1粗2扫、中矿合并返回流程处理,
与中矿顺序返回流程相比,在精矿硫品位略低的情况下硫回收率提高了1.7个百分点;将现场细粒浮
选2次扫选精矿合并给入粗粒浮硫扫选2作业,可提高硫回收率1.4个百分点,工业试验指标较好。

Abstract:

The sulfur grade of the first-stage cyclone overflow in the concentrator of Wushan Copper
Mine is 8.46%,and the particle size is extremely fine. The yield of -10 μm particle size is 44.93%,and the
sulfur distribution rate is 44.20%. In order to improve the effect of on-site fine sulfur recovery,a beneficia⁃
tion test was carried out. The results show that the suitable diameters of the overflow pipe and the grit nozzle
of the secondary classification cyclone are 48 mm and 20 mm respectively,and the sulfur distribution rate of
the secondary classification grit is 73.40%,which is 2.13 percentage points higher than that of the on-site
cyclone parameters. The total amount of collector ethyl xanthate determined by the test was 140 g/t,and the
corresponding amounts of roughing 1,scavenging 1 and scavenging 2 were 80,40 and 20 g/t,respectively.
The cyclone grading grits of the sample were treated by one roughing two scavenging and middling merging
and returning process. Compared with the middling sequential returning process,the sulfur recovery rate
was increased by 1.7 percentage points under the condition of slightly lower sulfur grade of the concentrate.
The on-site fine-grained flotation two-time scavenging concentrate is combined into the coarse-grained sul⁃
fur flotation two-time scavenging operation,which can increase the sulfur recovery rate by 1.4 percentage
points,and the industrial test index is good.

Key words: