欢迎访问《现代矿业》杂志官方网站,今天是 分享到:
×

扫码分享

现代矿业 ›› 2026, Vol. 42 ›› Issue (03): 76-81.

• 矿物加工工程 • 上一篇    下一篇

某硫化铅锌矿铅锌浮选分离试验研究

袁 锦1 赵冠飞2   

  1. 1. 深圳市中金岭南有色金属股份有限公司凡口铅锌矿;2. 江西理工大学资源与环境工程学院
  • 出版日期:2026-03-25 发布日期:2026-04-07

Experimental Study on Lead and Zinc Flotation Separation of a Lead-Zinc Sulfide Ore

  1. 1. Fankou Lead Zinc Mine,Shenzhen Zhongjin Lingnan Nonferrous Metals Co.,Ltd.; 2. College of Resources and Environmental Engineering,Jiangxi University of Science and Technology
  • Online:2026-03-25 Published:2026-04-07

摘要: 广东某硫化铅锌矿为了提高铅、锌浮选分离指标,针对铅、锌浮选分离困难的问题, 进行了铅、锌依次优先浮选流程试验。在降低矿浆 pH 值(pH 值由现场 12 降低至 10 左右)的情况 下,采用组合抑制剂硫酸锌+海藻酸钠,在原矿铅品位 4.58%、锌品位 9.33% 的基础上,最终得到了 铅品位 55.12%、铅回收率 86.05% 的铅精矿和锌品位 52.68%、锌回收率 95.37% 的锌精矿,试验指标 较好。接触角与 zeta电位测试结果表明:抑制剂硫酸锌+海藻酸钠在闪锌矿表面更容易吸附并改变 其疏水性,该组合抑制剂有望在实际生产中应用,可减少试验流程中的石灰用量,对保护环境具有 重要作用。

关键词: 方铅矿, 闪锌矿, 组合抑制剂, 浮选分离

Abstract: In order to improve the flotation separation index of lead and zinc in a lead-zinc sulfide ore in Guangdong,in view of the difficulty of flotation separation of lead and zinc,the test of lead and zinc in turn preferential flotation process is carried out.Under the condition of reducing the pH value of the pulp (the pH value is reduced from field 12 to about 10),the combined inhibitor zinc sulfate + sodium alginate is used. On the basis of the raw orelead grade of 4.58% and the zinc grade of 9.33%,the lead concentrate with lead grade of 55.12% and lead recovery of 86.05% and the zinc concentrate with zinc grade of 52.68% and zinc recovery of 95.37% are finally obtained. The test index is better.The contact angle and zeta poten‐ tial test results show that the inhibitor zinc sulfate + sodium alginate is easier to adsorb on the surface of sphalerite and change its hydrophobicity. The combined inhibitor is expected to be applied in actual pro‐ duction,which can reduce the amount of lime in the test process and play an important role in protecting the environment.

Key words: galena, sphalerite, combined inhibitors, flotation separation