强磁—浮选工艺回收攀西某选钛尾矿中钛铁矿试验*

为了回收攀西某钒钛磁铁矿选钛尾矿中钛铁矿,在试样化学成分分析、粒度分析的基
础上,采用强磁抛尾—分级磨矿除铁—除铁尾矿强磁精选—浮选精选工艺,获得了产率 4.13%、TiO2
品位47.15%,回收率30.71%的钛精矿。通过强磁选和浮选的联合使用,可以实现对选钛尾矿中钛铁
矿的高效回收,不仅提高了钛铁矿的回收率,而且提高了资源综合利用率,对于钛资源的可持续利用
具有重要意义,研究结果可为类似选钛尾矿的回收利用提供参考。

  

  1. 1. 攀钢集团矿业有限公司设计研究院;
    2. 钒钛资源综合利用国家重点实验室
  • 出版日期:2024-06-17 发布日期:2024-08-07

Test on Recovery of Ilmenite from a Titanium Tailings in Western Panzhihua
by High Intensity Magnetic Separation-Flotation Process

In order to recover ilmenite from titanium tailings of a vanadium-titanium magnetite ore in
Western Panzhihua,high-intensity magnetic discarding tailings-classification grinding iron removal-high-
intensity magnetic separation of iron removal tailings-flotation separation is carried out based on the chemi⁃
cal composition analysis and particle size analysis of the sample,a titanium concentrate withyield rate of
4.13%,TiO2 grade of 47.15% and recovery of 30.71% is obtained. Through the combined of high-intensity
magnetic separation and flotation,the efficient recovery of ilmenite in titanium tailings can be achieved,
which not only improves the recovery rate of ilmenite,but also improves the comprehensive utilization rate
of resources. It is of great significance for the sustainable utilization of titanium resources. The research re⁃
sults can provide reference for the recovery and utilization of similar titanium tailings.
#br#   

  1. 1. Design and Research Institute of Panzhihua Iron and Steel Group Mining Co.,Ltd.;
    2.State Key Laboratory for Comprehensive Utilization of Vanadium Titanium Resources
  • Online:2024-06-17 Published:2024-08-07

摘要:

为了回收攀西某钒钛磁铁矿选钛尾矿中钛铁矿,在试样化学成分分析、粒度分析的基
础上,采用强磁抛尾—分级磨矿除铁—除铁尾矿强磁精选—浮选精选工艺,获得了产率 4.13%、TiO2
品位47.15%,回收率30.71%的钛精矿。通过强磁选和浮选的联合使用,可以实现对选钛尾矿中钛铁
矿的高效回收,不仅提高了钛铁矿的回收率,而且提高了资源综合利用率,对于钛资源的可持续利用
具有重要意义,研究结果可为类似选钛尾矿的回收利用提供参考。

关键词:

Abstract:

In order to recover ilmenite from titanium tailings of a vanadium-titanium magnetite ore in
Western Panzhihua,high-intensity magnetic discarding tailings-classification grinding iron removal-high-
intensity magnetic separation of iron removal tailings-flotation separation is carried out based on the chemi⁃
cal composition analysis and particle size analysis of the sample,a titanium concentrate withyield rate of
4.13%,TiO2 grade of 47.15% and recovery of 30.71% is obtained. Through the combined of high-intensity
magnetic separation and flotation,the efficient recovery of ilmenite in titanium tailings can be achieved,
which not only improves the recovery rate of ilmenite,but also improves the comprehensive utilization rate
of resources. It is of great significance for the sustainable utilization of titanium resources. The research re⁃
sults can provide reference for the recovery and utilization of similar titanium tailings.

Key words: