河南栾川三道庄某低品位钨钼矿WO3品位为0.1%左右,钨主要以白钨矿形式存在,由
于钨的嵌布粒度较细,脉石矿物种类多,性质复杂,钨回收难度较高。针对该低品位矿进行钨回收试
验,在钨粗选阶段采用聚糖类有机抑制剂 LM 替代水玻璃,采用捕收性和选择性相对较好的捕收剂
ZF,并在钨精选阶段采用低模数水玻璃,减少了抑制剂消耗,最终从 WO3品位 0.097% 的给矿中获得
了WO3品位31.22%、回收率82.84%的钨精矿,实现了该低品位钨资源的高效浮选回收。
  

  1. 1. 中南大学资源加工与生物工程学院;
    2. 洛阳栾川钼业集团股份有限公司;
    3. 广东省科学院资源利用与稀土开发研究所
  • 出版日期:2024-04-15 发布日期:2024-08-13

Experimental Study on Tungsten Recovery from a Low-grade Tungsten-molybdenum Mine
in Sandaozhuang,Luanchuan County

A low-grade tungsten-molybdenum ore in Sandaozhuang,Luanchuan,Henan contains
about 0.1% WO3. Tungsten mainly exists in the form of scheelite. Due to the fine grain size of tungsten,the
variety and complex properties of gangue minerals,it is difficult to recover tungsten. The tungsten recovery
test was carried out for the low-grade ore. The polysaccharide organic inhibitor LM was used to replace the
sodium silicatein the tungsten roughing separation,and the collector ZF with relatively good collecting and
selectivity was used. The low modulus sodium silicate was used in the tungsten cleaning,which reduced the
consumption of the inhibitor. Finally,the tungsten concentrate with WO3 grade of 31.22% and recovery rate
of 82.84% was obtained from the feed ore with WO3 grade of 0.097 %,which realized the efficient flotation
recovery of the low-grade tungsten resource.
  

  1. 1. School of Resource Processing and Bioengineering,Central South University;
    2. CMOC Group Limited;
    3.Institute of Resource Utilization and Rare Earth Development,Guangdong Academy of Sciences
  • Online:2024-04-15 Published:2024-08-13

摘要:

河南栾川三道庄某低品位钨钼矿WO3品位为0.1%左右,钨主要以白钨矿形式存在,由
于钨的嵌布粒度较细,脉石矿物种类多,性质复杂,钨回收难度较高。针对该低品位矿进行钨回收试
验,在钨粗选阶段采用聚糖类有机抑制剂 LM 替代水玻璃,采用捕收性和选择性相对较好的捕收剂
ZF,并在钨精选阶段采用低模数水玻璃,减少了抑制剂消耗,最终从 WO3品位 0.097% 的给矿中获得
了WO3品位31.22%、回收率82.84%的钨精矿,实现了该低品位钨资源的高效浮选回收。

关键词:

Abstract:

A low-grade tungsten-molybdenum ore in Sandaozhuang,Luanchuan,Henan contains
about 0.1% WO3. Tungsten mainly exists in the form of scheelite. Due to the fine grain size of tungsten,the
variety and complex properties of gangue minerals,it is difficult to recover tungsten. The tungsten recovery
test was carried out for the low-grade ore. The polysaccharide organic inhibitor LM was used to replace the
sodium silicatein the tungsten roughing separation,and the collector ZF with relatively good collecting and
selectivity was used. The low modulus sodium silicate was used in the tungsten cleaning,which reduced the
consumption of the inhibitor. Finally,the tungsten concentrate with WO3 grade of 31.22% and recovery rate
of 82.84% was obtained from the feed ore with WO3 grade of 0.097 %,which realized the efficient flotation
recovery of the low-grade tungsten resource.