鲁南矿业公司尾矿回选试验

王坤胜1,邓庆山1,宋坤2,金子桥3   

  1. 1.莱钢鲁南矿业公司;2.山东兴盛矿业有限公司;3.山东省冶金设计院
  • 出版日期:2013-04-15 发布日期:2013-04-26

Tailings Re-concentration Tests for Lunan Mining Company

Wang Kunsheng1,Deng Qingshan1,Song Kun2,Jin Ziqiao3   

  1. 1.Lunan Mining Company, Laiwu Steel and Iron Group;2.Shandong Xingsheng Mining Co., Ltd.;3.Metallurgical Design Institute of Shandong Province
  • Online:2013-04-15 Published:2013-04-26

摘要: 针对莱钢鲁南矿业公司尾矿坝尾矿储量巨大且尾矿TFe含量较高(品位为15.02%),mFe为1.65%,回收价值巨大的情况,进行了再磨再选回收试验。试验结果表明:采用磨矿—磁粗选—再磨—磁选—反浮选的工艺流程可有效处理尾矿,最后获得了精矿铁品位为65.76%,产率为.5.50%,回收率为24.08%的满意指标,经济效益显著。

关键词: 贫磁铁矿, 尾矿再选, 磁选, 反浮选

Abstract: In view of huge reserves of tailings with high TFe content grading at 15.02% and mFe grade of 1.65% in tailings dam of Lunan Mining Company of Laiwu Steel & Iron Company, the re-grinding and re-concentration tests are carried out due to its huge recovery value. The test results show that the tailings are effectively treated by the process of grinding-coarse magnetic separation-regrinding-magnetic separation -reserve flotation. By this method, final concentrate with Fe grade of 65.76%, the yield of 5.50% and the recovery of 24.08% were obtained, which brings significant economic benefit.