微波辅助下萤石粉对含铁蛇纹石中镁的高效浸出研究

黄 巍 王本英 宋婉情 张子炫 黄瀚颉 谢蒙蒙   

  1. 沈阳化工大学环境与安全工程学院
  • 出版日期:2026-07-25 发布日期:2026-08-14

Study on Efficient Leaching of Magnesium from Iron-containing Serpentine by Fluorite Powder Under Microwave Assistance

HUANG Wei WANG Benying SONG Wanqing ZHANG Zixuan HUANG Hanjie XIE Mengmeng   

  1. College of Environmental and Safety Engineering,Shenyang University of Chemical Technology
  • Online:2026-07-25 Published:2026-08-14

摘要: 为进一步提升蛇纹石中有价组分的提取效果,以青海某选矿厂含铁蛇纹石尾矿为研 究对象,考察了在萤石粉做助浸剂条件下微波辅助作用对其中镁和铁浸出效果的影响。研究结果 表明:以萤石粉做助浸剂时,在微波时间 3 min、微波功率 400 W、浸出温度 70 ℃、浸出时间 30 min、 硫酸浓度 4.0 mol/L、萤石粉用量 3% 的浸出条件下,Mg 和 TFe 浸出率最佳,分别达到 97.02%、 50.90%;在此基础上,采用沉淀法对浸出液中的镁离子进行回收,调节浸出液 pH 值为 8.5,在 40 ℃ 条件下加热搅拌 25 min后,加入非离子型聚丙烯酰胺 0.05 g/L,轻微搅拌后静置 10 min并过滤,可将 硫酸镁粗溶液中的铁离子等杂质除去,其去除率为 99.84%;此后,在持续搅拌条件下继续调节滤液 pH 值为 11.0,静置陈化 60 min 后,可得到 Mg(OH)2粗产品,其纯度达到 95.73%,为蛇纹石尾矿的资 源化利用提供了新的技术路径。

关键词: 含铁蛇纹石尾矿, 浸出, 萤石助浸剂, 微波辅助, 氢氧化镁

Abstract: In order to further improve the extraction effect of valuable components in serpentine, taking the iron-bearing serpentine tailings of a concentrator in Qinghai as the research object,the effect of microwave-assisted action on the leaching of magnesium and iron under the condition of fluorite powder as leaching aid is investigated. The results show that when fluorite powder is used as leaching aid,the leaching rate of Mg and TFe is the best under the leaching conditions of microwave time 3 min,micro⁃ wave power 400 W,leaching temperature 70 ℃,leaching time 30 min,sulfuric acid concentration 4.0 mol/L and fluorite powder dosage 3%,reaching 97.02% and 50.90%,respectively.On this basis,the mag⁃ nesium ion in the leaching solution is recovered by precipitation method. The pH value of the leaching so⁃ lution is adjusted to 8.5. After heating and stirring at 40 ℃ for 25 min,0.05 g/L non-ionic polyacrylamide is added. After slight stirring,it is allowed to stand for 10 min and filter. The impurities such as iron ions in the crude solution of magnesium sulfate can be removed,and the removal rate is 99.84%.After that, the pH value of the filtrate is adjusted to 11.0 under continuous stirring conditions,and the crude product of Mg(OH)2 is obtained after static aging for 60 min. The purity of Mg(OH)2 reaches 95.73%,which pro⁃ vides a new technical path for the resource utilization of serpentine tailings.

Key words: iron-containing serpentine tailings, leaching, fluorite leaching aid agent, microwave as? sistance, magnesium hydroxide